Mechanical

Density: Gr./Cu. Cm. · 2.6-3.2
Lb./Cu. Ft. · 160-200
Hardness, Mohs 2.0-3.2
Cleavage Basal, Eminent
Crystal Structure Monoclinic
Max. Temperature with no decomposition 400-500°C
Specific heat (25°C) .206-.209
Thermal Conductivity perpendicular to cleavage: Cal./Sq. Cm./Sec./Cm./°C · 16x10-4
B.T.U./Sq. Ft./Hr./I.°F · 4.6
Coefficient of expansion per °C perpendicular to cleavage:   20° - 100° C · 15x10-6 - 25x10-6
100° - 300° C · 15x10-6 - 25x10-6
300° - 600° C · 16x10-6 - 36x10-6
Coefficient of expansion per °C parallel to cleavage:     0° - 200° C ·   8x10-6 - 9x10-6
200° - 500° C · 10x10-6 - 12x10-6
Tensile strength, P.S.I. 37,000 - 43,000
Modulus of elasticity 25x106

Electrical

Dielectric Constant 6.5 - 9
Dielectric Strength (highest qualities 1-3 mils thick), olts/Mil. 6,000 - 3,000
Power Factor at 25°C (77°F) (highest qualities), percent:       60 cycles · 0.08 - 0.09
1 megacycle · 0.01 - 0.02
Resistivity, Ohm-Cm. 1012 - 1015

Optical

Optic axial angle (2V) degrees 38 - 47
Orientation of optic plane to plane of symmetry Perpendicular
Indexes of refraction Alfa · 1.552 - 1.570
ß · 1.582 - 1.607
Char  · 1.588 - 1.611
*Muscovite
*Compiled by U.S. Bureau of Mines

Spruce Pine Mica Company
P.O. Box 219 · Spruce Pine, N. C.  28777
Phone (828) 765-4241

info@spruce-pine-mica.com

 

Home ] Natural Mica ] Mica Paper ] Plastics ] Glass Laminates ]